- 弯曲强度 [MPa]: 10.7
- 脆化温度 [℃]: -41.0
Physical Properties | Metric | English | Comments |
---|---|---|---|
Mooney Viscosity | 63 @Temperature 100 °C | 63 @Temperature 212 °F | ML 1 + 4 |
Mechanical Properties | Metric | English | Comments |
Hardness, Shore A | 64 | 64 | Vulcanizate, Press cured, TC95 +3min at 160°C |
Tensile Strength, Ultimate | 10.7 MPa | 1550 psi | Vulcanizate, Press cured, TC95 +3min at 160°C |
Elongation at Break | 301 % | 301 % | Vulcanizate, Press cured, TC95 +3min at 160°C |
50% Modulus | 0.00190 GPa | 0.276 ksi | Vulcanizate, Press cured, TC95 +3min at 160°C |
100% Modulus | 0.00400 GPa | 0.580 ksi | Vulcanizate, Press cured, TC95 +3min at 160°C |
200% Modulus | 0.00780 GPa | 1.13 ksi | Vulcanizate, Press cured, TC95 +3min at 160°C |
300% Modulus | 0.0103 GPa | 1.49 ksi | Vulcanizate, Press cured, TC95 +3min at 160°C |
Tear Strength | 26.0 kN/m | 148 pli | Die C, Vulcanizate, Press cured, TC95 +3min at 160°C |
Compression Set | 60 % @Temperature 125 °C | 60 % @Temperature 257 °F | Pellets cured MDR t'95 + 15 min, 70 hr; Method B |
Thermal Properties | Metric | English | Comments |
Brittleness Temperature | -41.0 °C | -41.8 °F | Temperature Retraction, TR-10 |