- 熔体流动速率 [g/10min]: 0.5
- 密度 [g/cm3]: 0.92
Physical Properties | Metric | English | Comments |
---|---|---|---|
Density | 0.920 g/cc | 0.0332 lb/in³ | ASTM D792 |
Thickness | 20.3 microns | 0.800 mil | |
Melt Flow | 0.50 g/10 min | 0.50 g/10 min | ASTM D1238 |
Antiblock Level | 5100 ppm | 5100 ppm | |
Slip Level | 900 ppm | 900 ppm | |
Mechanical Properties | Metric | English | Comments |
Film Tensile Strength at Yield, MD | 11.0 MPa | 1600 psi | ASTM D882 |
Film Tensile Strength at Yield, TD | 10.11 MPa | 1466 psi | ASTM D882 |
Film Elongation at Break, MD | 350 % | 350 % | ASTM D882 |
Film Elongation at Break, TD | 650 % | 650 % | ASTM D882 |
Impact | 9.5 | 9.5 | [lbf]; Puncture Resistance; Dow Method |
800 | 800 | [ft-lbf/in3]; Toughness MD; ASTM D882 | |
1000 | 1000 | [ft-lbf/in3]; Toughness TD; ASTM D882 | |
Elmendorf Tear Strength MD | 400 g | 400 g | ASTM D1922 |
Elmendorf Tear Strength TD | 700 g | 700 g | ASTM D1922 |
Elmendorf Tear Strength, MD | 19.7 g/micron | 500 g/mil | ASTM D1922 |
Elmendorf Tear Strength, TD | 34.4 g/micron | 875 g/mil | ASTM D1922 |
Dart drop Test | 500 g | 1.10 lb | Method A; ASTM D1709 |
Film Tensile Strength at Break, MD | 52.4 MPa | 7600 psi | ASTM D882 |
Film Tensile Strength at Break, TD | 45.96 MPa | 6666 psi | ASTM D882 |