- 密度 [g/cm3]: 1.29
- 吸水率 [%]: 0.14
- 缺口冲击强度: 1.71
- 断裂伸长率 [%]: 162
- 弯曲强度 [MPa]: 114.0
- 弯曲模量 [MPa]: 6.21
- 热变形温度 [℃]: 135.0
Physical Properties | Metric | English | Comments |
---|---|---|---|
Density | 1.29 - 1.39 g/cc | 0.0466 - 0.0502 lb/in³ | Average value: 1.34 g/cc Grade Count:7 |
Filler Content | 35.0 - 43.0 % | 35.0 - 43.0 % | Average value: 39.5 % Grade Count:4 |
Water Absorption | 0.140 - 1.50 % | 0.140 - 1.50 % | Average value: 0.697 % Grade Count:4 |
Linear Mold Shrinkage | 0.00100 - 0.00300 cm/cm | 0.00100 - 0.00300 in/in | Average value: 0.00180 cm/cm Grade Count:5 |
Mechanical Properties | Metric | English | Comments |
Tensile Strength, Ultimate | 114 - 140 MPa | 16500 - 20300 psi | Average value: 129 MPa Grade Count:7 |
Elongation at Break | 2.00 - 5.00 % | 2.00 - 5.00 % | Average value: 3.63 % Grade Count:7 |
Modulus of Elasticity | 7.58 - 13.3 GPa | 1100 - 1930 ksi | Average value: 9.64 GPa Grade Count:7 |
Flexural Yield Strength | 162 - 207 MPa | 23500 - 30000 psi | Average value: 184 MPa Grade Count:4 |
Flexural Modulus | 6.21 - 8.27 GPa | 900 - 1200 ksi | Average value: 7.41 GPa Grade Count:4 |
Izod Impact, Notched | 1.71 - 2.08 J/cm | 3.20 - 3.90 ft-lb/in | Average value: 1.94 J/cm Grade Count:4 |
Izod Impact, Unnotched | 9.08 - 11.2 J/cm | 17.0 - 21.0 ft-lb/in | Average value: 10.0 J/cm Grade Count:4 |
Charpy Impact Unnotched | 4.50 - 7.12 J/cm² | 21.4 - 33.9 ft-lb/in² | Average value: 6.16 J/cm² Grade Count:3 |
4.50 - 7.25 J/cm² @Temperature -30.0 - 30.0 °C | 21.4 - 34.5 ft-lb/in² @Temperature -22.0 - 86.0 °F | Average value: 6.21 J/cm² Grade Count:3 | |
Charpy Impact, Notched | 1.26 - 1.40 J/cm² | 6.00 - 6.66 ft-lb/in² | Average value: 1.31 J/cm² Grade Count:3 |
1.06 - 1.30 J/cm² @Temperature -30.0 - 30.0 °C | 5.04 - 6.19 ft-lb/in² @Temperature -22.0 - 86.0 °F | Average value: 1.14 J/cm² Grade Count:3 | |
Electrical Properties | Metric | English | Comments |
Electrical Resistivity | 1.00e+12 - 1.00e+14 ohm-cm | 1.00e+12 - 1.00e+14 ohm-cm | Average value: 5.27e+13 ohm-cm Grade Count:4 |
Thermal Properties | Metric | English | Comments |
CTE, linear | 20.0 - 32.4 µm/m-°C | 11.1 - 18.0 µin/in-°F | Average value: 27.5 µm/m-°C Grade Count:3 |
Deflection Temperature at 0.46 MPa (66 psi) | 135 - 177 °C | 275 - 350 °F | Average value: 165 °C Grade Count:4 |
Deflection Temperature at 1.8 MPa (264 psi) | 125 - 171 °C | 257 - 340 °F | Average value: 159 °C Grade Count:4 |
Flammability, UL94 | HB | HB | Grade Count:7 |
Processing Properties | Metric | English | Comments |
Processing Temperature | 216 - 266 °C | 420 - 510 °F | Average value: 241 °C Grade Count:3 |
Mold Temperature | 65.6 - 104 °C | 150 - 220 °F | Average value: 85.0 °C Grade Count:4 |
Injection Pressure | 68.9 - 103 MPa | 10000 - 15000 psi | Average value: 86.2 MPa Grade Count:4 |