- 弯曲模量 [MPa]: 7.00
Physical Properties | Metric | English | Comments | ||
---|---|---|---|---|---|
Specific Gravity | 1.82 g/cc | 1.82 g/cc | ISO 1183 | ||
Water Absorption | <= 0.30 % | <= 0.30 % | 23°C/24h | ||
Linear Mold Shrinkage | 0.0040 - 0.010 cm/cm | 0.0040 - 0.010 in/in | |||
Mechanical Properties | Metric | English | Comments | ||
Tensile Stress | 83.0 MPa | 12000 psi | |||
Elongation at Yield | 1.4 % | 1.4 % | |||
1.9 % | 1.9 % | flexural | |||
Modulus of Elasticity | 8.00 GPa | 1160 ksi | |||
Flexural Strength | 115 MPa | 16700 psi | |||
Flexural Modulus | 7.00 GPa | 1020 ksi | |||
Charpy Impact Unnotched | 2.00 J/cm² | 9.52 ft-lb/in² | edgewise; ISO 179 1eU | ||
Electrical Properties | Metric | English | Comments | ||
Surface Resistance | >= 1.00e+12 ohm | >= 1.00e+12 ohm | |||
Insulation Resistance | >= 1.00e+12 ohm | >= 1.00e+12 ohm | |||
Thermal Properties | Metric | English | Comments | ||
Thermal Conductivity | 0.600 W/m-K | 4.16 BTU-in/hr-ft²-°F | HOT-DISK || 60x60x3 mm | ||
Maximum Service Temperature, Air | 110 °C | 230 °F | |||
180 °C | 356 °F | short term | |||
Processing Properties | Metric | English | Comments | ||
Processing Temperature | 280 °C | 536 °F | mass temp | ||
Nozzle Temperature | 265 - 275 °C | 509 - 527 °F | |||
Zone 1 | 285 - 295 °C | 545 - 563 °F | |||
Zone 2 | 270 - 280 °C | 518 - 536 °F | |||
Zone 3 | 265 - 275 °C | 509 - 527 °F | |||
Mold Temperature | 60.0 - 120 °C | 140 - 248 °F | |||
Drying Temperature | 80.0 °C @Time 21600 - 28800 sec | 176 °F @Time 6.00 - 8.00 hour | |||
120 °C @Time 7200 - 18000 sec | 248 °F @Time 2.00 - 5.00 hour | Dehumidifying dryer | |||
Descriptive Properties | |||||
Color | silver grey |